摘要:To achieve the comprehensive utilization of solid waste and reduce costs, fly ash, carbide slag, and low-clinker cement were used to produce lightweight foamed concrete block. Granulated blast-furnace slag (GBFS) was used as composition correction material in the block. The effects of curing temperature and dosage of low-clinker cement on the performance of foamed concrete block were investigated. The optimal material proportioning is obtained: fly ash 58.5%, carbide slag 20%, GBFS 10%, gypsum 1.5% and low-clinker cement 10%. The proper curing regime is “temperature rising 4h-180°C constant temperature 4h-natural cooling”. The results indicate that the compressive strength of the block reaches 3.55 MPa while the density is 616.9 kg/m3. The performance of the product meets JC/T 1062-2007 (China professional standard of foamed concrete block).