摘要:This article lists three typical abnormal microstructures of overhead power line suspension clamps, including inclusion, flake graphite and cementite network. A series of tests including macro check, hardness measurement, composition tests, Energy-dispersive x-ray analysis and metallographic observation have been carried out. The experimental results showed that the causes of abnormal microstructures mainly include: high content of impurities, flake graphite blank and unfulfilled annealing heat treatment. It is suggested to strengthen the supervision on suspension clamps before using, and focus on the quality inspection of metallographic structure and composition.